{"id":4021,"date":"2021-12-17T10:45:31","date_gmt":"2021-12-17T09:45:31","guid":{"rendered":"http:\/\/www.woodresearch.sk\/cms\/?p=4021"},"modified":"2021-12-17T10:45:55","modified_gmt":"2021-12-17T09:45:55","slug":"surface-irregularities-of-oak-wood-after-transversal-cutting-with-a-circular-saw","status":"publish","type":"post","link":"https:\/\/www.woodresearch.sk\/cms\/surface-irregularities-of-oak-wood-after-transversal-cutting-with-a-circular-saw\/","title":{"rendered":"Surface irregularities of oak wood after transversal cutting with a circular saw"},"content":{"rendered":"\n<div class=\"wp-block-pdf-viewer-block-standard\" style=\"text-align:left\"><div class=\"uploaded-pdf\"><a href=\"https:\/\/www.woodresearch.sk\/cms\/wp-content\/uploads\/2021\/12\/Surface-irregularities-of-oak-wood-after-transversal-cutting-with-a-circular-saw.pdf\" data-width=\"\" data-height=\"\"><\/a><\/div><\/div>\n","protected":false},"excerpt":{"rendered":"<p>This paper deals with the effect of saw blade type (24, 40 and 60 teeth) and sawn distance on the primary profile (Pz) of tranvesre surface of European oak (Quercus robur L.) after transversal cutting. Transversal cutting was provided at constant cutting speed vc = 62 m.s-1 and with manual feeding using circular saw blade. An additional parameter was to determine the maximum sawn distance for each type of saw blade up to the point where the saw blade overheated, as well as the beginning of the blackening of the wood surface. The highest values of the primary profile (Pz) were achieved with a saw blade with 24 teeth, lower values were measured on wood cut with a 40 tooth blade and the lowest values after cutting with a 60 tooth blade. As the saw distance increased, there was no rapid and steep increase in the primary profile values, but these values gradually increased slightly, probably due to the gradual blunting of the tool.<\/p>\n","protected":false},"author":5,"featured_media":0,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[3719],"tags":[3734,3735,3733,3019,3736],"release_year":[],"ppma_author":[2024,2822],"class_list":["post-4021","post","type-post","status-publish","format-standard","hentry","category-wood-research-volume-66-number-6-2021","tag-circular-saw","tag-primary-profile-pz","tag-saw-blade","tag-surface-quality","tag-tranversal-cutting"],"featured_image_src":null,"author_info":{"display_name":"Stela Sl\u00e1mov\u00e1","author_link":"https:\/\/www.woodresearch.sk\/cms\/author\/slamovavupc-sk\/"},"authors":[{"term_id":2024,"user_id":0,"is_guest":1,"slug":"monika-sarvasova-kvietkova","display_name":"Monika Sarva\u0161ov\u00e1 Kvietkov\u00e1","avatar_url":"https:\/\/secure.gravatar.com\/avatar\/?s=96&d=mm&r=g","0":null,"1":"","2":"","3":"","4":"","5":"","6":"","7":"","8":""},{"term_id":2822,"user_id":0,"is_guest":1,"slug":"miroslav-gasparik","display_name":"Miroslav Ga\u0161par\u00edk","avatar_url":"https:\/\/secure.gravatar.com\/avatar\/?s=96&d=mm&r=g","0":null,"1":"","2":"","3":"","4":"","5":"","6":"","7":"","8":""}],"_links":{"self":[{"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/posts\/4021","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/users\/5"}],"replies":[{"embeddable":true,"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/comments?post=4021"}],"version-history":[{"count":2,"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/posts\/4021\/revisions"}],"predecessor-version":[{"id":4024,"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/posts\/4021\/revisions\/4024"}],"wp:attachment":[{"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/media?parent=4021"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/categories?post=4021"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/tags?post=4021"},{"taxonomy":"release_year","embeddable":true,"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/release_year?post=4021"},{"taxonomy":"author","embeddable":true,"href":"https:\/\/www.woodresearch.sk\/cms\/wp-json\/wp\/v2\/ppma_author?post=4021"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}